Next Article in Journal
Ecological and Health Risks Attributed to Rare Earth Elements in Coal Fly Ash
Next Article in Special Issue
Study on the Direct and Indirect Photolysis of Antibacterial Florfenicol in Water Using DFT/TDDFT Method and Comparison of Its Reactivity with Hydroxyl Radical under the Effect of Metal Ions
Previous Article in Journal
Biomonitoring of Oxidative-Stress-Related Genotoxic Damage in Patients with End-Stage Renal Disease
Previous Article in Special Issue
Degradation of Butylated Hydroxyanisole by the Combined Use of Peroxymonosulfate and Ferrate(VI): Reaction Kinetics, Mechanism and Toxicity Evaluation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Z-Type Heterojunction MnO2@g-C3N4 Photocatalyst-Activated Peroxymonosulfate for the Removal of Tetracycline Hydrochloride in Water

1
College of Resources and Environment Engineering, Shandong University of Technology, Zibo 255000, China
2
Department of Environmental Engineering, College of Biology and the Environment, Nanjing Forestry University, Nanjing 210037, China
3
Department of Marine Engineering, Jimei University, Xiamen 361021, China
4
Research Institute of Clean Chemical Technology, School of Chemistry and Chemical Engineering, Shandong University of Technology, Zibo 255049, China
*
Authors to whom correspondence should be addressed.
Toxics 2024, 12(1), 70; https://doi.org/10.3390/toxics12010070
Submission received: 10 November 2023 / Revised: 10 January 2024 / Accepted: 10 January 2024 / Published: 14 January 2024

Abstract

:
A Z-type heterojunction MnO2@g-C3N4 photocatalyst with excellent performance was synthesized by an easy high-temperature thermal polymerization approach and combined with peroxymonosulfate (PMS) oxidation technology for highly efficient degrading of tetracycline hydrochloride (TC). Analysis of the morphological structural and photoelectric properties of the catalysts was achieved through different characterization approaches, showing that the addition of MnO2 heightened visible light absorption by g-C3N4. The Mn1-CN1/PMS system showed the best degradation of TC wastewater, with a TC degradation efficiency of 96.97% following 180 min of treatment. This was an approximate 38.65% increase over the g-C3N4/PMS system. Additionally, the Mn1-CN1 catalyst exhibited excellent stability and reusability. The active species trapping experiment indicated •OH and SO4•− remained the primary active species to degrade TC in the combined system. TC degradation pathways and intermediate products were determined. The Three-Dimensional Excitation-Emission Matrix (3DEEM) was employed for analyzing changes in the molecular structure in TC photocatalytic degradation. The biological toxicity of TC and its degradation intermediates were investigated via the Toxicity Estimation Software Test (T.E.S.T.). The research offers fresh thinking for water environment pollution treatment.

1. Introduction

Tetracycline antibiotics are among the most frequently adopted antibiotics in livestock, aquaculture, and healthcare [1]. Tetracycline hydrochloride (TC), a tetracycline antibiotic, cannot be completely broken down in the environment because of its stable chemical properties [2]. The misuse and release of antibiotics in the ecosystem can promote the development of various drug-resistant bacteria and the enhancement of resistance genes [3], causing severe risk to global health and the ecosystem [4,5]. As a result, it is important to find a green, effective, and economical way to degrade TC effluent.
Currently, the commonly used remediation methods for environmental pollutants include adsorption [6], flocculation precipitation [7], ion exchange [8], and biochemical methods [9,10]. However, the above methods have the disadvantages of complicated procedures, high costs, and low removal efficiency. Advanced oxidation processes (AOPs) are considered a hopeful degradation technology because of their ability to generate highly reactive radicals, including hydroxyl radicals (•OH) and sulfate radicals (SO4•−) [11,12]. Interestingly, peroxymonosulfate (PMS)-based AOPs (PMS-AOPs) can produce SO4•− with higher redox potential, better selectivity, and a more comprehensive pH selection range [13]. The PMS could be excited by photocatalysis, carbon materials, and transition metal oxides to generate SO4•− [13,14,15,16,17]. Photocatalysis activation of PMS is one of the most widely used techniques because photocatalytic methods are inexpensive, simple, and efficient [18]. Many scholars have reported the effective degradation of pollutants by combining photocatalysts with PMS activation [15]. Liu et al. [19] found that the combination of graphitic carbon nitride (g-C3N4) nanosheets and PMS enhanced the removal of Bisphenol A under visible light, with complete removal in 90 min. Guan et al. [20] investigated whether the introduction of persulfate in the Co3O4/CeO2 system improved the removal efficacy of TC. Therefore, the combination of PMS and photocatalytic systems can effectively degrade antibiotic wastewater.
Recently, with good stability, reaction to light in the visible range, and unique properties of affordability, g-C3N4 has gained much attention as a non-metallic semiconductor material [21]. Meanwhile, research has now demonstrated that g-C3N4 can activate PMS to degrade organic pollutants [19]. Unfortunately, g-C3N4 still has significant limitations, including weak conductivity and quick recombination of photogenerated electron-holes (e-h+), which restricts its practical applicability in environmental purification [22]. Hence, numerous techniques have been developed for improving the photocatalytic activity of g-C3N4, involving metal or non-metal doping [23,24], construction nanostructures [25], and combinations of different semiconductors [26]. Among all modification methods, the combination of other semiconductors and g-C3N4 remains an excellent method for constructing Z-type heterojunction materials [27,28].
Transition metal oxide semiconductors can serve as catalysts and PMS activators to produce strongly oxidizing SO4•−. As a typical transition metal oxide, manganese dioxide (MnO2) has the benefits of low cost, environmental friendliness, and good conductivity [29]. MnO2 is an effective PMS activator due to the abundant oxygen mobility in the MnO2 lattice and the electron transfer between Mn species [30,31]. Therefore, the addition of MnO2 to g-C3N4 for forming a Z-type heterojunction is a viable approach for improving photocatalytic performance of the catalyst [32,33].
In our research, a MnO2@g-C3N4 heterojunction with a Z-type structure was prepared for efficient TC photocatalytic degradation with PMS and visible light. Various characterization approaches were employed for analyzing the morphology, chemical compositions, and optoelectronic properties of samples. The photocatalytic degradation performance of TC was studied under diverse reaction environment parameters. Meanwhile, the intermediates of TC and possible reaction pathways were determined. The Toxicity Estimation Software Test (T.E.S.T.) was employed for assessing TC toxicity and its intermediates. The average TC removal rate observed under the current procedures at the wastewater treatment plants was 96.97%. This research presents a safe, green, and environmentally friendly treatment method for purifying and treating antibiotic wastewater.

2. Experimental Section

2.1. Materials

The chemical reagents used in our research are all listed in Supplementary file Text 1.

2.2. Photocatalyst Sample Preparation

2.2.1. Preparation of g-C3N4

The g-C3N4 preparation had two steps. In the first step, bulk g-C3N4 was produced through thermal polycondensation [34]. A total of 5 g of melamine was laid in a muffle furnace, with the temperature heated to 550 °C at 5 °C min−1 and held for 4 h. After cessation of heating, the yellowish solid was ground for 30 min to form a fine powder. To pyrolytically peel the prepared bulk g-C3N4 into thinner g-C3N4, in the second step, the yellowish g-C3N4 powder was divided into several portions, and the g-C3N4 was laid in crucible and placed in a muffle furnace, with the temperature heated to 500 °C at 10 °C min−1 within 2 h to obtain g-C3N4.

2.2.2. Preparation of MnO2

MnO2 was synthesized by redox coprecipitation using MnCl2-4H2O and KMnO4 (molar ratio 3:2). The brown precipitate was separated by adding KMnO4 solution (2 mol L−1 100 mL) to MnCl2 solution (3 mol L−1 100 mL) dropwise at 5 mL min−1 during magnetic stirring and drying for 4 h at 90 °C. The solution was stirred again to redissolve the dried powder in water. The precipitate was washed properly with alcohol by filtration and dried for 12 h at 90 °C to obtain MnO2.

2.2.3. Preparation of MnO2@g-C3N4

Three mass ratios of MnO2 and g-C3N4 (MnO2:g-C3N4 = 1:2, 1:1, and 2:1) were weighed and were recorded as Mn1-CN2, Mn1-CN1, and Mn2-CN1, respectively. The mixture was ground for 30 min to form a fine powder and then laid in crucible in a muffle furnace, with the temperature heated to 400 °C at 5 °C min−1 within 4 h and chilled to normal temperature to obtain Mn-CN photocatalytic composite materials with different ratios.

2.3. Photocatalyst Characterization

The morphology and dimensions of the photocatalysts were identified using scanning electron microscopy (SEM) techniques. X-ray diffraction (XRD) patterns were obtained using a Brucker D8 Advance diffraction apparatus. The surface chemistry of the samples was characterized by X-ray photoelectron spectroscopy (XPS). Solid-state UV-Vis diffuse reflectance spectroscopy (UV-Vis-DRS) was used to study the optical properties and separation of photogenerated electrons and holes. Electrochemical impedance spectroscopy (EIS) was measured using a CHI 660B electrochemical system. The degradation intermediates of TC were analyzed by HPLC-MS. The molecular structural changes during TC degradation were analyzed using Three-Dimensional Excitation-Emission Matrix (3DEEM). The parameters used for all characterizations are given in Supplementary file Text 2.

2.4. Photocatalytic Degradation of TC by Mn-CN

In the experiments, the photocatalytic degradation performance of the catalysts was tested via a dominant wavelength of 400 nm and a 300 W solar simulator xenon lamp (xenon lamp model and manufacturer’s declared spectrum as well as photocatalytic device diagram are shown in Supplementary Figure S1). The photocatalyst (0.03 g) was dispersed into 50 mL of 20 mg L−1 TC solution for each experiment. The solution was stirred for 30 min without light until adsorption equilibrium was reached. Then, 0.6 mM PMS was added, and the lamp was switched on. Samples were taken every 30 min during the photocatalytic process. Supernatant measurement was performed with UV-Vis spectrophotometer (UV-5100B) at 357 nm after filtration through a 0.22 μm microfilter membrane.

3. Results and Discussion

3.1. Properties of the Material

Figure 1 displays the SEM and TEM pictures of the samples. The g-C3N4 was composed of many irregular lamellar and layered structures [35], with a large specific surface area, as shown in Figure 1a [36]. MnO2 exhibited regular small particle-size nanospheres with a rough surface but a relatively uniform particle size distribution (Figure 1b). Moreover, MnO2 was dispersed on the g-C3N4 layered structure in Mn1-CN1 (Figure 1c). Figure 1d–f shows the TEM images of the sample. Many MnO2 particles were found on the g-C3N4 surface, indicating that the composites of MnO2 and g-C3N4 were well prepared [37]. As depicted in Figure 1g–j, C, N, O, and Mn were evenly scattered on the Mn1-CN1 surface. The percentages of C, N, O and Mn in Mn1-CN1 were 50.36%, 16.42%, 6.05%, and 27.17%, respectively (Figure 1k). Figure 1l shows the HRTEM image of Mn1-CN1; two different types of lattice stripes can be found from the (002) and (111) facets of the crystal structure at crystallographic plane distances of approximately 0.34 and 0.24 nm, respectively.
Figure 2a displays the XRD patterns of g-C3N4, MnO2, and Mn1-CN1. The g-C3N4 and Mn1-CN1 have the same peaks located at 13.1° and 27.4° [38]. The diffraction peak at 13.1° was weak and belonged to the (100) crystal plane of g-C3N4, which was made up of repeating structural units of the heptazine ring. The diffraction peak at 27.4° was strong and belonged to the g-C3N4 (002) crystal plane. This indicates that the sample was a lamellar stacking of graphite-like material [39]. The location and intensity of MnO2 diffraction peaks were relatively uniform and smooth, with the diffraction peaks at 2θ = 12.7°, 25.2°, 37.1°, and 66.0° for lattice planes (001), (002), (111), and (311), respectively [40]. The relatively weak intensity and broad peak pattern of these diffraction peaks indicated that the product was a compact growth of amorphous and weakly crystalline MnO2. Furthermore, all prominent peaks of g-C3N4 and MnO2 could be seen in the Mn1-CN1 spectra, which indicates that MnO2 was compounded into g-C3N4 to form Mn1-CN1.
Figure 2b displays the FT-IR of the sample. The peak of g-C3N4 at around 807.50 cm−1 can be related to the triazinic moiety [41]. Vibrational absorption peaks at 1252.82 and 1623.35 cm−1 correspond to the vibrational stretch of the carbon and nitrogen bonds (C-N and C=N). The stretching vibrations of -NH2 and -NH groups and of the -OH bond correspond to the peak at 3151.74 cm−1 [42]. The characteristic peak of MnO2 was mainly at 530.32 cm−1. The positions of the Mn1-CN1 absorption peaks were essentially the same as those of MnO2 and g-C3N4 absorption peaks, illustrating that the MnO2 had been loaded onto g-C3N4.
Samples’ N2 adsorption-desorption isotherms and pore-size profiles were measured, with the results shown in Figure 2c,d. The specific surface area of Mn1-CN1 was 90.99 m2g−1, which was 5.6 and 3.8 times higher relative to g-C3N4 and MnO2, respectively. Due to the large number of MnO2 particles tightly dispersed on the surface of g-C3N4, the specific surface area of the composites was enlarged relative to single g-C3N4 and MnO2, which contributed to TC degradation. Under the International Union of Pure and Applied Chemistry (IUPAC) classification, all three samples displayed the Type IV isotherm of the H3 type, indicating that narrow pores existed, unique to mesoporous materials, in the prepared samples [43]. From Figure 2d, the pore size distribution curves of all photocatalysts, g-C3N4, MnO2, and Mn1-CN1, indicate a mesoporous structure. Moreover, the pore volume of Mn1-CN1 was also greater relative to g-C3N4 and MnO2. The larger specific surface area and higher porosity of the catalyst could increase the contact area of active molecules and pollutants, thus enhancing photocatalytic performance [44].
The UV-Vis DRS spectrum shows the optical properties of samples (Figure 2e). The G-C3N4 sample absorbed light within the range of 450 nm to UV. Compared with g-C3N4, MnO2 exhibited strong absorption in the wavelength range of 300–800 nm. Notably, the introduction of MnO2 resulted in a significant red-shift of Mn1-CN1, indicating that the MnO2 was able to extend the absorption range of Mn1-CN1 for visible light [45]. The bandgap energy of the samples was calculated via the Kubelka–Munk function [46], as shown below:
( α h v ) 1 / 2 = K h v E g
where α, v, h, K, and Eg are absorbance, photon frequency, Planck’s constant, proportional constant, and bandgap energy, respectively. This can be derived from the diffuse reflectance spectra after Tauc fitting with Eg values of 2.67 eV and 1.71 eV for g-C3N4 and MnO2 samples, respectively (Figure 2f). Valence bands (VB) of g-C3N4 and MnO2 can be estimated from the XPS valence band spectra (Supplementary Figure S2), with positions of 1.54 and 2.34 eV, respectively. The conduction band (CB) position was calculated via Equation (2), and the CB potentials of g-C3N4 and MnO2 were −1.13 and 0.63 eV, respectively.
E C B = E V B E g
Figure 3a displays the total XPS spectra of the photocatalysts. The XPS spectrum of Mn1-CN1 contained peaks of C 1s and N 1s elements in g-C3N4 and peaks of Mn 2p and O 1s elements in MnO2. In addition, no peaks of other elements were found in the Mn1-CN1 catalyst, indicating that the composite was not doped with impurities of other elements. Figure 3b shows the three peaks obtained by fitting the C 1s high resolution spectrum with the XPSPEAK software. The three peaks at 284.2, 285.2, and 287.4 eV resulted from the C-C bond, C=N bond, and N=C-N2 group, respectively [47]. In Figure 3c, the four characteristic peaks of N 1s spectra at 397.8, 398.7, 400.2, and 403.8 eV originated from the C=N-C bond of sp2-hybridized aromatic nitrogen, (C)3-N2 bond of the sp2-hybridized bridged nitrogen atom, C-N-H of the sp3-hybridized terminal functional group [48,49], and the charge effect of the π-excited states [50], respectively. These results prove the existence of the graphite phase g-C3N4. The two characteristic peaks in Mn 2p spectra (Figure 3d) at 642.0 and 654.0 eV corresponded to the binding energy spin-orbit double peaks of Mn 2p3/2 and Mn 2p1/2, respectively, which is consistent with the nature of MnO2. In addition, the change in the valence of Mn was crucial for the photocatalytic reaction. The presence of characteristic peaks at 652.9 and 641.4 eV indicates that both Mn3+ and Mn4+ were present in MnO2. As shown in the O 1s spectra (Figure 3e), the three peaks at 529.1, 530, and 531.1 eV were due to the atomic lattice oxygen of MnO2, hydroxyl groups attached to the Mn surface, and adsorbed oxygen [51].
In addition, the interfacial charge transfer of the samples was studied using the EIS technique. Photoelectric performance tests were performed on a CHI 660B electrochemical system. The system used a standard three-electrode system with a photocatalyst as the working electrode, a Pt plate counter electrode and an Ag/AgCl reference electrode, and Na2SO4 as the electrolyte solution. The smaller arc radius of the EIS curve indicates lower resistance of the sample and a better electron-hole pair separation [52]. From Figure 3f, it can be seen that the electrochemical impedance arc radius of Mn1-CN1 was significantly smaller relative to g-C3N4 and MnO2, indicating that Mn1-CN1 possessed the smallest charge transfer resistance and quicker interfacial charge transfer efficiency. The above results show that the formation of heterojunctions could speed up the transfer of photo-excited electron-hole pairs, which improved photocatalytic degradation [28].

3.2. Photocatalytic Efficiency of the Samples toward TC Degradation

From Figure 4a, it can be seen that the Mn-CN/PMS system exhibited excellent degradation performance, with a degradation efficiency of 85.06%. When MnO2 was introduced, g-C3N4/MnO2 samples displayed excellent photocatalytic degradation efficiency for TC, which resulted from the formation of the g-C3N4/MnO2 heterojunction. However, degradation efficiency of TC for the sole MnO2 system was less than 7.0%. Moreover, the TC degradation efficiency for the sole g-C3N4 or PMS system was also relatively low, with only 15.5% and 5.4% removal, respectively. When both Mn-CN and PMS were present, the TC degradation efficiency reached 85.06%, suggesting that PMS was activated by the Mn-CN activator.
The photocatalytic degradation performance of different Mn-CN catalysts is shown in Figure 4b. Compared with other samples, the Mn1-CN1 catalysts exhibited better degradation performance. TC degradation efficiency achieved 85.06% when PMS existed after 180 min. However, when the MnO2 ratio increased, the TC degradation efficiency did not significantly change because the excessive MnO2 increased the absorption and scattering of photons, which affected light utilization by g-C3N4 and reduced photocatalytic efficiency. This is consistent with previous reports [23].

3.3. The Effect of Catalyst Dosage

TC degradation efficiency was enhanced when the amount of the Mn1-CN1 catalyst increased (Figure 4c). When the Mn1-CN1 catalyst was dosed from 0.2 to 0.6 g L−1, TC degradation efficiency improved from 54.3% to 85.06%. With the increase in the amount of the Mn1-CN1 catalyst, the number of active sites increased, which was helpful for improving TC photocatalytic degradation efficiency [26]. However, TC degradation efficiency was not significantly improved by more than 1% when the Mn1-CN1 dose reached 0.8 g L−1. When the amount of the Mn1-CN1 catalyst was too high, the excessive Mn1-CN1 impeded the passage of light, further affecting the number of photogenerated electron-hole pairs generated by the photocatalyst and causing the degradation efficiency of TC solution to decrease.

3.4. The Effect of initial TC Concentration

As Figure 4d displays, as the TC concentration was augmented from 10 to 25 mg L−1, the TC degradative efficiency diminished from 99.1% to 77.9% in 180 min photoreaction. When the catalyst and the PMS dosage were constant, the electron-hole pairs produced were almost constant, and the number of active molecules produced by the photocatalytic system tended to be constant. The photocatalytic system was able to provide sufficient active substances while the initial TC concentration was 10 mg L−1. Therefore, each TC molecule was more easily oxidized, improving the utilization rate of the active species. The photocatalytic system provided insufficient active species, and TC degradation efficiency diminished, with gradual augmentation of the initial TC concentration. In addition, the amount of intermediate products produced in TC degradation also increased with the initial TC concentration. This could result in occupation of other active sites [28].

3.5. The Effect of PMS Dosage on TC Degradation

The influence of different PMS concentrations on TC degradation is detailed in Figure 4e. As the PMS dosage was augmented, the TC degradation efficiency was gradually enhanced. The photocatalytic degradation efficiency of TC increased from 64.7% to 85.06% when the concentration of PMS was increased from 0.2 to 0.6 mM, which was attributed to the production of more reactive oxygen species by Mn1-CN1 [53]. However, the TC degradation capacity was not significantly improved when PMS was dosed to 0.8 mM, with no great improvement in TC degradation efficiency. Excess PMS could react with SO4•−, forming persulfate radicals (S2O82−), which have a much lower oxidation capacity than SO4•− (see Equations (3) and (4)) [54].
SO 4 + S 2 O 8 2     S 2 O 8 + SO 4   2
SO 4 + SO 4     S 2 O 8 2

3.6. The Effect of Initial Solution pH

The influence of diverse initial solution pH levels on TC degradation is detailed in Figure 4f. In acidic conditions, the combined system showed better degradation performance, whereas in alkaline conditions, a lower TC degradation efficiency remained. The TC degradation efficiency obtained was 96.97% at a pH of 3, while the lowest degradation efficiency was recorded when the pH was 11 (50.6%). When the solution pH was below the equipotential point of Mn1-CN1 in the acidic environment, the Mn1-CN1 catalyst was positively charged [55]. This could promote the migration of photoexcited electrons to the catalyst surface and effectively lessen the compounding of e and h+, thus enhancing the catalytic efficiency of the catalyst. The Mn1-CN1 was negatively charged in an alkaline environment, which did not assist the transfer of photoexcited electrons to the catalyst surface, thus affecting photocatalytic efficiency.
Supplementary Figure S3 exhibits the UV-visible degradation spectra for each of the influencing factors. The intensity of the typical absorption peaks decreased as the photocatalytic reaction progressed. This indicated that the Mn1-CN1/PMS system produced effective active species. The reaction kinetic rate constant for TC degradation can be calculated from the first-order kinetic equation (Equation (5)), where k and t are the degradation rate constant and reaction time (min), respectively, Ct is the TC concentration at t min (mg L−1), and C0 is the initial TC concentration (mg L−1).
l n C t / C 0 = k t
The photocatalytic process of MnO2/g-C3N4 was compared with other g-C3N4-based photocatalysts reported in the literature (Table 1). The findings proved that MnO2/g-C3N4 exhibited relatively better photocatalytic activity for organic pollutant removal. In addition, the kinetic diagrams at the TC level for each of the above influences are detailed as Supplementary Figure S4a–f, showing first-order reaction kinetics well explained the TC degradation rate, and the Mn1-CN1/PMS system had a high degradation rate constant (Supplementary Table S1).
The TOC analyzer (Analytickjena, multi N/C 2100s) was used to determine the change in total organic carbon in the TC solution. As shown in Figure 5, the removal of TOC increased with increasing of the photocatalytic treatment time. When the time was 180 min, the removal rate of TOC was 81.3%. This indicates that the Mn1-CN1/PMS system has significant photocatalytic treatment ability under visible light, which can oxidize industrial recalcitrant pollutants such as TC.

3.7. Stability of Photocatalytic Materials

As illustrated in Figure 6a, there was no appreciable difference between the first used catalyst and the five recycled ones, and TC degradation efficiency only declined from 96.5% to 91.7%. The decrease in TC degradation efficiency could be explained by the accumulation of intermediates on the Mn1-CN1 catalyst, which competed with the photocatalyst active site, and the loss of a small amount of photocatalyst during the cycling process experiments [63]. Meanwhile, to further confirm the stability, Mn1-CN1 was analyzed by SEM/TEM, XPS, and XRD after five cyclic experiments. The SEM/TEM image (Supplementary Figure S5) shows no great changes in Mn1-CN1 morphology. The XRD pattern (Supplementary Figure S6) shows that the diffraction peaks were significantly unchanged after the reaction. Furthermore, the XPS spectra of the recovered Mn1-CN1 were similar to those of the original catalyst, indicating that the surface structure of the sample did not change after five cycles of reaction (Supplementary Figure S7). The Mn1-CN1 composite photocatalyst was prepared with high stability, which is very useful for practical applications in wastewater treatment.

3.8. Visible Light Photocatalytic Degradation Mechanism

The active species trapping experiment was performed to investigate the active species involved in TC degradation [64,65]. Reagents IPA, BQ, EDTA-2Na, and MA were employed for capturing •OH, superoxide radical (•O2), h+, and SO4•−, respectively. Supplementary Figure S8 shows the addition of IPA and MA significantly inhibited TC degradation efficiency, which diminished from 97% to 41.08% and 54.9%, correspondingly, revealing that •OH and SO4•− were primary active species. Additionally, the presence of BQ also inhibited TC degradation efficiency, suggesting that •O2 was also involved in the photocatalytic reaction. However, EDTA-2Na only slightly inhibited TC photodegradation, revealing that h+ was not the major active substance.
The possible mechanism of the degrading of TC pollutants by the Mn1-CN1/PMS system under visible light was investigated (Figure 6b). Unlike the type II configuration, the Z-type MnO2/g-C3N4 photocatalyst combines a semiconductor of high energy in the valence band (MnO2) with another semiconductor of lower bandgap and stronger reduction ability in the conduction band (g-C3N4). The electrons photogenerated in the MnO2 are cross-combined with the holes of the g-C3N4. This process yields the accumulation of separated charge carriers in the respective phases. The MnO2’s holes keep their strong oxidation ability, while the g-C3N4’s electrons retain their reduction potential. In Z-scheme heterojunction photocatalysts, the Mn1-CN1 generated photo-induced e and h+ (Equation (6)) were excited under visible light irradiation. Recombination reactions are conducted by photogenerated e in the CB of MnO2 and h+ in the VB of g-C3N4. The H2O or OH could be oxidized by h+ on the VB of MnO2 to produce •OH (Equations (7) and (8)). Photogenerated e on the CB of g-C3N4 reacted with dissolved oxygen, forming •O2 (Equation (9)). Meanwhile, the PMS received photogenerated e, which can be activated for producing SO4•− (Equation (10)). The SO4•− was able to react rapidly with OH for producing •OH (Equation (11)). The SO4•− and •OH were vital for TC degradation (Equation (12)). Overall, ideal matching of the energy band structure between g-C3N4 and MnO2 can increase the amount of photogenerated e and h+ [66].
  MnO 2 @ g - C 3 N 4 + h v     e + h +
H 2 O + h +       OH + H +
  OH + h + OH
O 2 + e O 2
HS O 5 + e OH + SO 4
SO 4 + OH OH + SO 4   2
OH + SO 4 + TC Degradation   products
Intermediates of TC degradation were identified by HPLC/MS for future investigation of the TC degradation mechanism. More information on the nine main intermediates can be found in Supplementary Table S2. Three possible transformation reactions, hydroxylation, carboxylation, and N-C bond cleavage, are shown in Figure 7 [67,68,69]. Since -C=C- was conjugated to the oxygen on the adjacent -OH, P1 (m/z = 461) and P2 (m/z = 476) were derived from the hydroxyl addition of two enol groups. The -OH served as an electron-donating group, weakening the -C=C- linkage, and was attacked by •OH, generating ketone and epoxide group transformations. Meanwhile, P1 was susceptible to attack by reactive radicals and further formation of polyhydroxylated P2 (m/z = 476) because of low electron density of the C(1)=C(2) bond of P1. The C(3)-N bond of P2 was then oxidized for producing P3 (m/z = 447). Finally, P4 (m/z = 495) was obtained through ring-opening the aromatic ring on P3. In degradation pathway 2, the TC molecule underwent deamidation under the attack of reactive radicals for producing P5 (m/z = 401). P6 (m/z = 417) was formed by -OH addition to the deamidated C1. P7 (m/z = 360) was an intermediate product formed when -OH and -CH3 on C5 of P6 were attacked by h+ and •O2 reactive oxide species, which were followed by dimethylamino and ring opening. In degradation pathway 3, the carbocyclic branched chain of P5 was destroyed by strong oxidizing radicals to produce P8 (m/z = 306). Finally, P8 underwent deacylation and demethylation dehydroxylation reactions to give P9 (m/z = 227). These intermediates were unstable and quickly oxidized to CO2 and H2O. A comparison of the by-products produced with the study of Yu et al. [28] revealed that the present study produced lesser quantities of by-products. This indicates that the Mn1-CN1/PMS system has significant photocatalytic treatment ability under visible light.
Supplementary Figure S9 shows Three-Dimensional Excitation-Emission Matrix (3DEEM) of TC at different photocatalytic times. The fluorescence peak of TC mainly occurred in the wavelength range of Ex/Em= (290–340 nm)/(380–460 nm), suggesting that TC was an aromatic protein-like compound. The intensity of the fluorescence peaks decreased with prolonged photocatalytic reaction time, suggesting that the aromatic benzene ring structure was damaged by the attack of the reactive species. The prominence peak almost disappeared after 180 min, suggesting that the simple aryl ring of TC was almost entirely disrupted (Supplementary Figure S8d).

3.9. TC Degradation Toxicity Analysis

To examine the environmental toxicity of TC, toxicity evaluation of the degradation products was used for contaminant status assessment. The biological toxicity of TC and its degradation intermediates were investigated via T.E.S.T. according to the quantitative structure–activity relationship (QSAR). Figure 8a,b shows the predicted values of daphnia magna LC50 and the developmental toxicity of the intermediates. The LC50-48 h values of most degradation intermediates were higher than that of TC, suggesting that TC was slowly transformed into less toxic intermediates. The products P2, P4, and P8 can be regarded as non-toxicants in Figure 8b. In addition, the results on the basis of bioaccumulation factors and mutagenicity illustrated that the photocatalytic reaction reduced the ecosystem hazard of TC and its intermediates [70]. Therefore, TC oxidation by Mn1-CN1/PMS system could reduce the toxicity of TC.

4. Conclusions

In this study, a Z-type Mn-CN heterojunction composite photocatalyst with excellent performance was successfully prepared by coupling the g-C3N4 with MnO2 via high-temperature thermal polymerization. The XRD, SEM, and TEM analysis showed synthesized Mn1-CN1 had good purity and a crystalline state. The catalytic experiments indicated that the Mn1-CN1/PMS system was the most effective, with the degradation efficiency of TC reaching 96.97% after 180 min of treatment, which was 38.65% higher relative to the g-C3N4/PMS system. The photocatalyst displayed marvelous stability and reusability after five cycle experiments. In addition, the PMS played an essential role in removing TC, while Mn1-CN1 was also an efficient activator for PMS under visible light irradiation. The active species trapping experiment showed •OH and SO 4 were major active species. Nine primary degradation intermediates and three possible degradation pathways were put forward. Toxicological evaluation of TC and its intermediates showed that the Mn1-CN1/PMS system could diminish TC toxicity. The findings showed the Mn1-CN1/PMS system was advantageous for the photocatalytic degradation of TC, which can offer potential application for the treatment of antibiotics in wastewater.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/toxics12010070/s1, Figure S1: (a) Spectrogram of the xenon lamp light source BBZM−Ⅲ, (b) Diagram of the photo-catalytic device; Figure S2: the XPS valence band spectra; Figure S3: The UV absorption spectra of TC degradation under optimal reaction conditions for each influencing factor. (a) Mn1−CN1 photocatalyst, the amount of Mn1−CN1 photocatalyst dosed was 0.6 g L–1, the dosage of PMS was 0.6 mM; (b) The initial concentration of TC was 10 mg L–1; (c) The initial pH was 3; Figure S4: (a) Catalyst type on the reaction kinetics of TC; (b) Reaction kinetics of different ratios of Mn−CN catalysts for the degradation of TC; (c) Reaction kinetics of catalyst dosing for degradation of TC; (d) Reaction ki-netics of TC degradation at initial TC concentrations; (e) Kinetics of PMS dosage in response to TC; (f) Initial pH on the reaction kinetics of TC; Figure S5: SEM (a) and TEM (b) images of the Mn1−CN1 cycle after reaction; Figure S6: The XRD patterns of Mn1−CN1 before and after reaction; Figure S7: XPS spectra of Mn1−CN1 after reaction: full spectrum (a), C 1s (b), N 1s (c), Mn 2p (d), O1s (e); Figure S8: Active species trapping experiments of as−prepared Mn1−CN1 for TC degra-dation under visible light irradiation. [IPA, BQ, EDTA−2Na] = 1 mM L–1, [MA] = 10 mM L–1. The experimental conditions: [photocatalyst] = 0.6 g L–1, [TC] = 20 mg L–1, [PMS] = 0.6 mM, pH = 7, time=180 min, and T = 25 °C; Figure S9: 3DEEM spectra of TC solutions after different treatment times: (a) 0 min; (b) 60 min; (c) 120 min; (d) 180 min; Table S1: Reaction rate constants for each influencing factor.; Table S2: The TC degradation intermediates detected by HPLC−MS.

Author Contributions

G.L.: conceptualization, investigation, data curation, formal analysis, writing—original draft, visualization. X.L.: data curation, resources. P.L.: methodology, conceptualization. H.G.: investigation. Z.W.: methodology, investigation. Q.Z.: writing—review and editing, validation. Y.L.: formal analysis. W.S.: supervision. J.A.: writing—review and editing, funding acquisition. Z.Z.: writing—review and editing. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by Natural Science Foundation of China (21706149 and 22006069); Natural Science Foundation of Shandong Province (ZR2023MB052).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data will be made available on request.

Acknowledgments

We would like to express our gratitude to the members of the Analysis and Testing Center of Shandong University of Technology and the School of Chemistry and Chemical Engineering for their technical assistance and suggestions.

Conflicts of Interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

References

  1. Wang, H.B.; Hu, C.; Liu, L.Z.; Xing, X.C. Interaction of ciprofloxacin chlorination products with bacteria in drinking water distribution systems. J. Hazard. Mater. 2017, 339, 174–181. [Google Scholar] [CrossRef] [PubMed]
  2. Wang, L.P.; Yang, G.P.; Wang, D.; Lu, C.Y.; Guan, W.S.; Li, Y.L.; Deng, J.; Crittenden, J. Fabrication of the flower-flake-like CuBi2O4/Bi2WO6 heterostructure as efficient visible-light driven photocatalysts: Performance, kinetics and mechanism insight. Appl. Surf. Sci. 2019, 495, 143521. [Google Scholar] [CrossRef]
  3. Li, J.N.; Cheng, W.X.; Xu, L.K.; Jiao, Y.N.; Baig, S.A.; Chen, H. Occurrence and removal of antibiotics and the corresponding resistance genes in wastewater treatment plants: Effluents’ influence to downstream water environment. Environ. Sci. Pollut. Res. 2016, 23, 6826–6835. [Google Scholar] [CrossRef] [PubMed]
  4. Moradi, S.; Sobhgol, S.A.; Hayati, F.; Isari, A.A.; Kakavandi, B.; Bashardoust, P.; Anvaripour, B. Performance and reaction mechanism of MgO/ZnO/Graphene ternary nanocomposite in coupling with LED and ultrasound waves for the degradation of sulfamethoxazole and pharmaceutical wastewater. Sep. Purif. Technol. 2020, 251, 117373. [Google Scholar] [CrossRef]
  5. Mirzaei, A.; Yerushalmi, L.; Chen, Z.; Haghighat, F. Photocatalytic degradation of sulfamethoxazole by hierarchical magnetic ZnO@g-C3N4: RSM optimization, kinetic study, reaction pathway and toxicity evaluation. J. Hazard. Mater. 2018, 359, 516–526. [Google Scholar] [CrossRef] [PubMed]
  6. Yang, G.R.; Gao, Q.Z.; Yang, S.Y.; Yin, S.H.; Cai, X.; Yu, X.Y.; Zhang, S.S.; Fang, Y.P. Strong adsorption of tetracycline hydrochloride on magnetic carbon-coated cobalt oxide nanoparticles. Chemosphere 2020, 239, 124831. [Google Scholar] [CrossRef] [PubMed]
  7. Yang, Z.; Jia, S.Y.; Zhuo, N.; Yang, W.B.; Wang, Y.P. Flocculation of copper(II) and tetracycline from water using a novel pH- and temperature-responsive flocculants. Chemosphere 2015, 141, 112–119. [Google Scholar] [CrossRef]
  8. Meng, X.; Liu, Z.M.; Deng, C.; Zhu, M.F.; Wang, D.Y.; Li, K.; Deng, Y.; Jiang, M.M. Microporous nano-MgO/diatomite ceramic membrane with high positive surface charge for tetracycline removal. J. Hazard. Mater. 2016, 320, 495–503. [Google Scholar] [CrossRef]
  9. Shao, S.C.; Wu, X.W. Microbial degradation of tetracycline in the aquatic environment: A review. Crit. Rev. Biotechnol. 2020, 40, 1010–1018. [Google Scholar] [CrossRef]
  10. Zhang, X.L.; Chen, J.X.; Li, J. The removal of microplastics in the wastewater treatment process and their potential impact on anaerobic digestion due to pollutants association. Chemosphere 2020, 251, 126360. [Google Scholar] [CrossRef]
  11. Khan, A.; Zhang, K.K.; Taraqqi-A-Kamal, A.; Wang, X.G.; Chen, Y.; Zhang, Y.R. Degradation of antibiotics in aqueous media using manganese nanocatalyst-activated peroxymonosulfate. J. Colloid Interface Sci. 2021, 599, 805–818. [Google Scholar] [CrossRef] [PubMed]
  12. Nguyen, T.B.; Huang, C.P.; Doong, R.A.; Wang, M.H.; Chen, C.W.; Dong, C.D. Manipulating the morphology of 3D flower-like CoMn2O4 bimetallic catalyst for enhancing the activation of peroxymonosulfate toward the degradation of selected persistent pharmaceuticals in water. Chem. Eng. J. 2022, 436, 135244. [Google Scholar] [CrossRef]
  13. Gao, Y.; Wang, Q.; Ji, G.Z.; Li, A.M. Degradation of antibiotic pollutants by persulfate activated with various carbon materials. Chem. Eng. J. 2022, 429, 132387. [Google Scholar] [CrossRef]
  14. Zhang, Y.; Zhou, J.B.; Chen, X.; Wang, L.; Cai, W.Q. Coupling of heterogeneous advanced oxidation processes and photocatalysis in efficient degradation of tetracycline hydrochloride by Fe-based MOFs: Synergistic effect and degradation pathway. Chem. Eng. J. 2019, 369, 745–757. [Google Scholar] [CrossRef]
  15. Chen, G.Y.; Yu, Y.; Liang, L.; Duan, X.G.; Li, R.; Lu, X.K.; Yan, B.B.; Li, N.; Wang, S.B. Remediation of antibiotic wastewater by coupled photocatalytic and persulfate oxidation system: A critical review. J. Hazard. Mater. 2021, 408, 124461. [Google Scholar] [CrossRef]
  16. Adil, S.; Maryam, B.; Kim, E.J.; Dulova, N. Individual and simultaneous degradation of sulfamethoxazole and trimethoprim by ozone, ozone/hydrogen peroxide and ozone/persulfate processes: A comparative study. Environ. Res. 2020, 189, 109889. [Google Scholar] [CrossRef]
  17. Ji, Y.F.; Dong, C.X.; Kong, D.Y.; Lu, J.H.; Zhou, Q.S. Heat-activated persulfate oxidation of atrazine: Implications for remediation of groundwater contaminated by herbicides. Chem. Eng. J. 2015, 263, 45–54. [Google Scholar] [CrossRef]
  18. Li, L.; Yuan, X.P.; Zhou, Z.P.; Tang, R.D.; Deng, Y.C.; Huang, Y.; Xiong, S.; Su, L.; Zhao, J.; Gong, D.X. Research progress of photocatalytic activated persulfate removal of environmental organic pollutants by metal and nonmetal based photocatalysts. J. Clean. Prod. 2022, 372, 133420. [Google Scholar] [CrossRef]
  19. Liu, B.C.; Qiao, M.; Wang, Y.B.; Wang, L.J.; Gong, Y.; Guo, T.; Zhao, X. Persulfate enhanced photocatalytic degradation of bisphenol A by g-C3N4 nanosheets under visible light irradiation. Chemosphere 2017, 189, 115–122. [Google Scholar] [CrossRef]
  20. Guan, R.P.; Yuan, X.Z.; Wu, Z.B.; Jiang, L.B.; Zhang, J.; Li, Y.F.; Zeng, G.M.; Mo, D. Efficient degradation of tetracycline by heterogeneous cobalt oxide/cerium oxide composites mediated with persulfate. Sep. Purif. Technol. 2019, 212, 223–232. [Google Scholar] [CrossRef]
  21. Jia, J.; Zhang, Q.Q.; Li, K.K.; Zhang, Y.T.; Liu, E.Z.; Li, X. Recent advances on g-C3N4-based Z-scheme photocatalysts: Structural design and photocatalytic applications. Int. J. Hydrogen Energy 2022, 48, 196–231. [Google Scholar] [CrossRef]
  22. Jiang, L.B.; Yuan, X.Z.; Zeng, G.M.; Liang, J.; Chen, X.H.; Yu, H.B.; Wang, H.; Wu, Z.B.; Zhang, J.; Xiong, T. In-situ synthesis of direct solid-state dual Z-scheme WO3/g-C3N4/Bi2O3 photocatalyst for the degradation of refractory pollutant. Appl. Catal. B Environ. 2018, 227, 376–385. [Google Scholar] [CrossRef]
  23. Song, Y.L.; Qi, J.Y.; Tian, J.Y.; Gao, S.S.; Cui, F.Y. Construction of Ag/g-C3N4 photocatalysts with visible-light photocatalytic activity for sulfamethoxazole degradation. Chem. Eng. J. 2018, 341, 547–555. [Google Scholar] [CrossRef]
  24. Guo, F.; Li, M.Y.; Ren, H.J.; Huang, X.L.; Shu, K.K.; Shi, W.L.; Lu, C.Y. Facile bottom-up preparation of Cl-doped porous g-C3N4 nanosheets for enhanced photocatalytic degradation of tetracycline under visible light. Sep. Purif. Technol. 2019, 228, 115770. [Google Scholar] [CrossRef]
  25. Gao, X.X.; Yang, B.Z.; Yao, W.Q.; Wang, Y.J.; Zong, R.L.; Wang, J.; Li, X.C.; Jin, W.J.; Tao, D.P. Enhanced photocatalytic activity of ZnO/g-C3N4 composites by regulating stacked thickness of g-C3N4 nanosheets. Environ. Pollut. 2020, 257, 113577. [Google Scholar] [CrossRef]
  26. Wang, J.J.; Tang, L.; Zeng, G.M.; Deng, Y.C.; Liu, Y.N.; Wang, L.G.; Zhou, Y.Y.; Guo, Z.; Wang, J.J.; Zhang, C. Atomic scale g-C3N4/Bi2WO6 2D/2D heterojunction with enhanced photocatalytic degradation of ibuprofen under visible light irradiation. Appl. Catal. B Environ. 2017, 209, 285–294. [Google Scholar] [CrossRef]
  27. Xue, S.Y.; Wu, C.Z.; Pu, S.Y.; Hou, Y.Q.; Tong, T.; Yang, G.; Qin, Z.J.; Wang, Z.M.; Bao, J.M. Direct Z-Scheme charge transfer in heterostructured MoO3/g-C3N4 photocatalysts and the generation of active radicals in photocatalytic dye degradations. Environ. Pollut. 2019, 250, 338–345. [Google Scholar] [CrossRef]
  28. Yu, H.B.; Wang, D.Y.; Zhao, B.; Lu, Y.; Wang, X.H.; Zhu, S.Y.; Qin, W.C.; Huo, M.X. Enhanced photocatalytic degradation of tetracycline under visible light by using a ternary photocatalyst of Ag3PO4/AgBr/g-C3N4 with dual Z-scheme heterojunction. Sep. Purif. Technol. 2020, 237, 116365. [Google Scholar] [CrossRef]
  29. Eslami, A.; Hashemi, M.; Ghanbari, F. Degradation of 4-chlorophenol using catalyzed peroxymonosulfate with nano-MnO2/UV irradiation: Toxicity assessment and evaluation for industrial wastewater treatment. J. Clean. Prod. 2018, 195, 1389–1397. [Google Scholar] [CrossRef]
  30. Jawad, A.; Zhan, K.; Wang, H.B.; Shahzad, A.; Zeng, Z.H.; Wang, J.; Zhou, X.Q.; Ullah, H.; Chen, Z.L.; Chen, Z.Q. Tuning of Persulfate Activation from a Free Radical to a Nonradical Pathway through the Incorporation of Non-Redox Magnesium Oxide. Environ. Sci. Technol. 2020, 54, 2476–2488. [Google Scholar] [CrossRef]
  31. Li, J.N.; Li, X.Y.; Wang, X.; Zeng, L.B.; Chen, X.; Mu, J.C.; Chen, G.H. Multiple regulations of Mn-based oxides in boosting peroxymonosulfate activation for norfloxacin removal. Appl. Catal. A Gen. 2019, 584, 117170. [Google Scholar] [CrossRef]
  32. Zhang, Q.; Peng, Y.; Deng, F.; Wang, M.; Chen, D.Z. Porous Z-scheme MnO2/Mn-modified alkalinized g-C3N4 heterojunction with excellent Fenton-like photocatalytic activity for efficient degradation of pharmaceutical pollutants. Sep. Purif. Technol. 2020, 246, 116890. [Google Scholar] [CrossRef]
  33. Nguyen, M.D.; Nguyen, T.B.; Tran, L.H.; Nguyen, T.G.; Fatimah, I.; Kuncoro, E.P.; Doong, R.A. Z-scheme S, B co-doped g-C3N4 nanotube@MnO2 heterojunction with visible-light-responsive for enhanced photodegradation of diclofenac by peroxymonosulfate activation. Chem. Eng. J. 2023, 452, 139249. [Google Scholar] [CrossRef]
  34. Dong, F.; Zhao, Z.W.; Xiong, T.; Ni, Z.L.; Zhang, W.D.; Sun, Y.J.; Ho, W.K. In Situ Construction of g-C3N4/g-C3N4 Metal-Free Heterojunction for Enhanced Visible-Light Photocatalysis. ACS Appl. Mater. Interfaces 2013, 145, 11392–11401. [Google Scholar] [CrossRef] [PubMed]
  35. Wang, Y.Z.; Yu, J.Y.; Peng, W.D.; Tian, J.; Yang, C. Novel multilayer TiO2 heterojunction decorated by low g-C3N4 content and its enhanced photocatalytic activity under UV, visible and solar light irradiation. Sci. Rep. 2019, 9, 5932. [Google Scholar] [CrossRef]
  36. Du, X.R.; Zou, G.J.; Wang, Z.H.; Wang, X.L. A scalable chemical route to soluble acidified graphitic carbon nitride: An ideal precursor for isolated ultrathin g-C3N4 nanosheets. Nanoscale 2015, 7, 8701–8706. [Google Scholar] [CrossRef]
  37. Panimalar, S.; Uthrakumar, R.; Selvi, E.T.; Gomathy, P.; Inmozhi, C.; Kaviyarasu, K.; Kennedy, J. Studies of MnO2/g-C3N4 hetrostructure efficient of visible light photocatalyst for pollutants degradation by sol-gel technique. Surf. Interfaces 2020, 20, 100512. [Google Scholar] [CrossRef]
  38. Bai, X.J.; Yan, S.C.; Wang, J.J.; Li, W.; Jiang, W.J.; Wu, S.L.; Sun, C.P.; Zhu, Y.F. A simple and efficient strategy for the synthesis of a chemically tailored g-C3N4 material. J. Mater. Chem. A 2014, 2, 17521–17529. [Google Scholar] [CrossRef]
  39. Liu, X.M.; Liu, Y.; Zhang, W.K.; Zhong, Q.Y.; Ma, X.Y. In situ self-assembly of 3D hierarchical 2D/2D CdS/g-C3N4 hereojunction with excellent photocatalytic performance. Mat. Sci. Semicon. Proc. 2020, 105, 104734. [Google Scholar] [CrossRef]
  40. Rivera-Lugo, Y.Y.; Félix-Navarro, R.M.; Trujillo-Navarrete, B.; Reynoso-Soto, E.A.; Silva-Carrillo, C.; Cruz-Gutiérrez, C.A.; Quiroga-González, E.; Calva-Yáez, J.C. Flower-like δ-MnO2 as cathode material of Li-ion batteries of high charge-discharge rates. Fuel 2021, 287, 119463. [Google Scholar] [CrossRef]
  41. Shen, G.D.; Pu, Y.P.; Cui, Y.F.; Jing, P.P. Easy synthesis of TiO2/g-C3N4 Heterostructure Photocatalyst with Large Surface Area and Excellent Photocatalytic Activity. Ceram. Int. 2017, 43, S664–S670. [Google Scholar] [CrossRef]
  42. Dai, X.; Xie, M.L.; Meng, S.G.; Fu, X.L.; Chen, S.F. Coupled systems for selective oxidation of aromatic alcohols to aldehydes and reduction of nitrobenzene into aniline using CdS/g-C3N4 photocatalyst under visible light irradiation. Appl. Catal. B Environ. 2014, 158, 382–390. [Google Scholar] [CrossRef]
  43. Yu, J.G.; Wang, S.H.; Cheng, B.; Zhang, L.; Huang, F. Noble metal-free Ni(OH)2-g-C3N4 composite photocatalyst with enhanced visible-light photocatalytic H2-production activity. Catal. Sci. Technol. 2013, 3, 1782–1789. [Google Scholar] [CrossRef]
  44. Zhang, Q.K.; Han, F.X.; Yan, Y.H.; Dai, Q.L.; Proctor, G.; Cheah, P.; Avijit, P.; Chandra, R.P.; Kang, N.; Hu, M.G.; et al. Preparation and properties of visible light responsive RGO/In2 TiO5 nanobelts for photocatalytic degradation of organic pollutants. Appl. Surf. Sci. 2019, 485, 547–553. [Google Scholar] [CrossRef]
  45. Nanda, B.; Pradhan, A.C.; Parida, K.M. A comparative study on adsorption and photocatalytic dye degradation under visible light irradiation by mesoporous MnO2 modified MCM-41 nanocomposite. Micropor. Mesopor. Mat. 2016, 226, 229–242. [Google Scholar] [CrossRef]
  46. Zhang, Y.G.; Wu, M.Y.; Kwok, Y.H.; Wang, Y.F.; Zhao, W.; Zhao, X.L.; Huang, H.B.; Leung, D.Y.C. In-situ synthesis of heterojunction TiO2/MnO2 nanostructure with excellent performance in vacuum ultraviolet photocatalytic oxidation of toluene. Appl. Catal. B Environ. 2019, 259, 118034. [Google Scholar] [CrossRef]
  47. Zhu, B.C.; Xia, P.F.; Ho, W.K.; Yu, J.G. Isoelectric point and adsorption activity of porous g-C3N4. Appl. Surf. Sci. 2015, 344, 188–195. [Google Scholar] [CrossRef]
  48. Wu, W.T.; Zhang, J.Q.; Fan, W.Y.; Li, Z.T.; Wang, L.Z.; Li, X.M.; Wang, Y.; Wang, R.Q.; Zheng, J.T.; Wu, M.B.; et al. Remedying Defects in Carbon Nitride to Improve both Photooxidation and H2 Generation Efficiencies. ACS Catal. 2016, 6, 3365–3371. [Google Scholar] [CrossRef]
  49. Lin, L.H.; Ou, H.H.; Zhang, Y.F.; Wang, X.C. Tri-s-triazine-Based Crystalline Graphitic Carbon Nitrides for Highly Efficient Hydrogen Evolution Photocatalysis. ACS Catal. 2016, 6, 3921–3931. [Google Scholar] [CrossRef]
  50. Qiu, P.X.; Chen, H.; Xu, C.M.; Zhou, N.; Jiang, F.; Wang, X.; Fu, Y.S. Fabrication of an exfoliated graphitic carbon nitride as a highly active visible light photocatalyst. J. Mater. Chem. A 2015, 3, 24237–24244. [Google Scholar] [CrossRef]
  51. Zhao, J.H.; Nan, J.; Zhao, Z.W.; Li, N.; Liu, J.; Cui, F.Y. Energy-efficient fabrication of a novel multivalence Mn3O4-MnO2 heterojunction for dye degradation under visible light irradiation. Appl. Catal. B Environ. 2017, 202, 509–517. [Google Scholar] [CrossRef]
  52. Li, B.X.; Shao, X.K.; Liu, T.X.; Shao, L.Z.; Zhang, B.S. Construction of metal/WO2.72/rGO ternary nanocomposites with optimized adsorption, photocatalytic and photoelectrochemical properties. Appl. Catal. B Environ. 2016, 198, 325–333. [Google Scholar] [CrossRef]
  53. Wang, Y.W.; Xiang, L.R.; Li, Z.; Han, J.G.; Guo, H. Sulfite activation by water film dielectric barrier discharge plasma for ibuprofen degradation: Efficiency, comparison of persulfate, mechanism, active substances dominant to pathway, and toxicity evaluation. Sep. Purif. Technol. 2024, 330, 125531. [Google Scholar] [CrossRef]
  54. Forouzesh, M.; Ebadi, A.; Aghaeinejad-Meybodi, A. Degradation of metronidazole antibiotic in aqueous medium using activated carbon as a persulfate activator. Sep. Purif. Technol. 2019, 210, 145–151. [Google Scholar] [CrossRef]
  55. Huang, D.L.; Li, J.; Zeng, G.M.; Xue, W.J.; Chen, S.; Li, Z.H.; Deng, R.; Yang, Y.; Cheng, M. Facile construction of hierarchical flower-like Z-scheme AgBr/Bi2WO6 photocatalysts for effective removal of tetracycline: Degradation pathways and mechanism. Chem. Eng. J. 2019, 375, 121991. [Google Scholar] [CrossRef]
  56. Ding, C.M.; Zhu, Q.R.; Yang, B.; Petropoulos, E.; Xue, L.H.; Feng, Y.F.; He, S.Y.; Yang, L.Z. Efficient photocatalysis of tetracycline hydrochloride (TC-HCl) from pharmaceutical wastewater using AgCl/ZnO/g-C3N4 composite under visible light: Process and mechanisms. J. Environ. Sci. 2023, 126, 249–262. [Google Scholar] [CrossRef] [PubMed]
  57. Zhao, W.; Li, Y.J.; Zhao, P.S.; Zhang, L.L.; Dai, B.L.; Xu, J.M.; Huang, H.B.; He, Y.L.; Dennis, Y.C. Novel Z-scheme Ag-C3N4/SnS2 plasmonic heterojunction photocatalyst for degradation of tetracycline and H2 production. Chem. Eng. J. 2021, 405, 126555. [Google Scholar] [CrossRef]
  58. Zhu, X.; Wang, Y.T.; Guo, Y.; Wan, J.Z.; Yan, Y.; Zhou, Y.X.; Sun, C. Environmental-friendly synthesis of heterojunction photocatalysts g-C3N4/BiPO4 with enhanced photocatalytic performance. Appl. Surf. Sci. 2021, 544, 148872. [Google Scholar] [CrossRef]
  59. Jing, H.C.; Ou, R.P.; Yu, H.B.; Zhao, Y.H.; Lu, Y.; Huo, M.X.; Huo, H.L.; Wang, X.Z. Engineering of g-C3N4 nanoparticles/WO3 hollow microspheres photocatalyst with Z-scheme heterostructure for boosting tetracycline hydrochloride degradation. Sep. Purif. Technol. 2021, 255, 117646. [Google Scholar] [CrossRef]
  60. Zhao, W.; Li, J.; She, T.T.; Ma, S.S.; Cheng, Z.P.; Wang, G.X.; Zhao, P.S.; Wei, W.; Xia, D.H.; Dennis, Y.C. Study on the Photocatalysis Mechanism of the Z-Scheme Cobalt Oxide Nanocubes/Carbon Nitride Nanosheets Heterojunction Photocatalyst with High Photocatalytic Performances. J. Hazard. Mater. 2021, 402, 123839. [Google Scholar] [CrossRef]
  61. Du, C.Y.; Zhang, Z.; Tan, S.Y.; Yu, G.L.; Chen, H.; Zhou, L.; Yu, L.; Su, Y.H.; Zhang, Y.; Deng, F.F.; et al. Construction of Z-scheme g-C3N4 / MnO2 /GO ternary photocatalyst with enhanced photodegradation ability of tetracycline hydrochloride under visible light radiation. Environ. Res. 2021, 200, 111427. [Google Scholar] [CrossRef] [PubMed]
  62. Xue, W.J.; Huang, D.L.; Li, J.; Zeng, G.M.; Deng, R.; Yang, Y.; Chen, S.; Li, Z.H.; Gong, X.M.; Li, B. Assembly of AgI nanoparticles and ultrathin g-C3N4 nanosheets codecorated Bi2WO6 direct dual Z-scheme photocatalyst: An efficient, sustainable and heterogeneous catalyst with enhanced photocatalytic performance. Chem. Eng. J. 2019, 373, 1144–1157. [Google Scholar] [CrossRef]
  63. Nguyen, M.D.; Nguyen, T.B.; Thamilselvan, A.; Nguyen, T.G.; Kuncoro, E.P.; Doong, R.A. Fabrication of visible-light-driven tubular F, P-codoped graphitic carbon nitride for enhanced photocatalytic degradation of tetracycline. J. Environ. Chem. Eng. 2021, 10, 106905. [Google Scholar] [CrossRef]
  64. Su, Y.Y.; Yang, Y.X.; Jiang, W.X.; Han, J.G.; Guo, H. A novel strategy of peracetic acid activation by dielectric barrier discharge plasma for bisphenol a degradation: Feasibility, mechanism and active species dominant to degradation pathway. Chem. Eng. J. 2023, 476, 146469. [Google Scholar] [CrossRef]
  65. Jiang, W.X.; Han, J.G.; Guo, H. Highlight the plasma-generated reactive oxygen species (ROSs) dominant to degradation of emerging contaminants based on experiment and density functional theory. Sep. Purif. Technol. 2024, 330, 125309. [Google Scholar] [CrossRef]
  66. Kaviyarasu, K.; Magdalane, C.M.; Manikandan, E.; Jayachandran, M.; Maaza, M. Well-Aligned Graphene Oxide Nanosheets Decorated with Zinc Oxide Nanocrystals for High Performance Photocatalytic Application. Int. J. Nanosci. 2015, 14, 8064. [Google Scholar] [CrossRef]
  67. Khan, M.H.; Bae, H.K.; Jung, J.Y. Tetracycline degradation by ozonation in the aqueous phase: Proposed degradation intermediates and pathway. J. Hazard. Mater. 2010, 181, 659–665. [Google Scholar] [CrossRef]
  68. Song, C.; Guo, B.B.; Sun, X.F.; Wang, S.G.; Li, Y.T. Enrichment and degradation of tetracycline using three-dimensional graphene/MnO2 composites. Chem. Eng. J. 2019, 358, 1139–1146. [Google Scholar] [CrossRef]
  69. Cheng, J.; Xie, Y.R.; Wei, Y.; Xie, D.R.; Sun, W.B.; Zhang, Y.; Li, M.H.; An, J.T. Degradation of tetracycline hydrochloride in aqueous via combined dielectric barrier discharge plasma and Fe–Mn doped AC. Chemosphere 2022, 286, 131841. [Google Scholar] [CrossRef]
  70. Ren, J.Y.; Song, H.Z.; Guo, H.; Yao, Z.Z.; Wei, Q.; Jiao, K.Q.; Li, Z.Y.; Zhong, C.C.; Wang, J.; Zhen, Y.Z. Removal of chloramphenicol in water by an improved water falling film dielectric barrier discharge reactor: Performance, mechanism, degradation pathway and toxicity evaluation. J. Clean. Prod. 2021, 325, 129332. [Google Scholar] [CrossRef]
Figure 1. SEM and TEM pictures of (a,d) g-C3N4, (b,e) MnO2, (c,f) Mn1-CN1; (gj) elemental mapping images of C, N, O, and Mn in Mn1-CN1; (k) EDS spectrum of Mn1-CN1; (l) HRTEM image of Mn1-CN1.
Figure 1. SEM and TEM pictures of (a,d) g-C3N4, (b,e) MnO2, (c,f) Mn1-CN1; (gj) elemental mapping images of C, N, O, and Mn in Mn1-CN1; (k) EDS spectrum of Mn1-CN1; (l) HRTEM image of Mn1-CN1.
Toxics 12 00070 g001
Figure 2. (a) XRD patterns (The hearts and clubs in 2a are the locations of the g−C3N4 and MnO2 characteristic peaks, respectively), (b) FT-IR spectra, (c) N2 adsorption-desorption isotherm curve, (d) pore size distribution of g-C3N4, MnO2, and Mn1-CN1, (e) UV-vis DRS spectra of the samples, (f) diffuse reflectance spectra after Tauc fitting for the different photocatalysts.
Figure 2. (a) XRD patterns (The hearts and clubs in 2a are the locations of the g−C3N4 and MnO2 characteristic peaks, respectively), (b) FT-IR spectra, (c) N2 adsorption-desorption isotherm curve, (d) pore size distribution of g-C3N4, MnO2, and Mn1-CN1, (e) UV-vis DRS spectra of the samples, (f) diffuse reflectance spectra after Tauc fitting for the different photocatalysts.
Toxics 12 00070 g002
Figure 3. Extended range XPS spectra of g-C3N4, MnO2, and Mn1-CN1 (a); high-resolution XPS patterns of C 1s (b), N 1s (c), Mn 2p (d), and O 1s (e); electrochemical impedance spectra (f).
Figure 3. Extended range XPS spectra of g-C3N4, MnO2, and Mn1-CN1 (a); high-resolution XPS patterns of C 1s (b), N 1s (c), Mn 2p (d), and O 1s (e); electrochemical impedance spectra (f).
Toxics 12 00070 g003
Figure 4. Photocatalytic degradation efficiency of (a) the different photocatalysts, (b) Mn-CN in different proportions, (c) amounts of the photocatalyst, (d) initial TC concentration, (e) PMS dosage, and (f) initial pH. The reaction conditions: [TC] = 20 mg L−1, [photocatalyst] = 0.6 g L−1, [PMS] = 0.6 mM, T = 25 °C, and pH = 7.
Figure 4. Photocatalytic degradation efficiency of (a) the different photocatalysts, (b) Mn-CN in different proportions, (c) amounts of the photocatalyst, (d) initial TC concentration, (e) PMS dosage, and (f) initial pH. The reaction conditions: [TC] = 20 mg L−1, [photocatalyst] = 0.6 g L−1, [PMS] = 0.6 mM, T = 25 °C, and pH = 7.
Toxics 12 00070 g004
Figure 5. TOC removal by Mn1-CN1/PMS system for TC photocatalytic degradation. Reaction conditions: TC = 20 mg L−1; photocatalyst = 0.6 g L−1; PMS = 0.6 mM; T = 25 °C; and pH = 7.
Figure 5. TOC removal by Mn1-CN1/PMS system for TC photocatalytic degradation. Reaction conditions: TC = 20 mg L−1; photocatalyst = 0.6 g L−1; PMS = 0.6 mM; T = 25 °C; and pH = 7.
Toxics 12 00070 g005
Figure 6. (a) Recyclability of Mn1-CN1 catalyst; (b) photocatalytic mechanism scheme of Mn1-CN1 composites.
Figure 6. (a) Recyclability of Mn1-CN1 catalyst; (b) photocatalytic mechanism scheme of Mn1-CN1 composites.
Toxics 12 00070 g006
Figure 7. Three possible degradation pathways of TC in the Mn1-CN1/PMS system.
Figure 7. Three possible degradation pathways of TC in the Mn1-CN1/PMS system.
Toxics 12 00070 g007
Figure 8. Toxicity analysis of reaction products: (a) The Daphnia magna LC50-48 h, (b) Developmental toxicity, (c) Bioaccumulation factors, (d) Mutagenicity.
Figure 8. Toxicity analysis of reaction products: (a) The Daphnia magna LC50-48 h, (b) Developmental toxicity, (c) Bioaccumulation factors, (d) Mutagenicity.
Toxics 12 00070 g008
Table 1. Comparison of TC degradation efficiencies with other C3N4-based photocatalysts.
Table 1. Comparison of TC degradation efficiencies with other C3N4-based photocatalysts.
Photocatalyst (g L−1)TC Concentration
(mg L−1)
Light Source TypeVolumes TestedTime (min)Removal (%)References
AgCl/ZnO/g-C3N4 (1.0)20 mg L−1400–700 nm40 ml80 min92.7%[56]
Ag-C3N4/SnS2 (0.4)15 mg L−1500 W Xe lamp50 ml150 min94.9%[57]
g-C3N4/BiPO4 (1.0)20 mg L−11000 W Xe lamp50 ml180 min97%[58]
C3N4/WO3 (0.4)10 mg L−1500 W Xe lamp (320–780nm)100 ml180 min79.8%[59]
Co3O4/g-C3N4 (0.4)15 mg L−1500 W Xe lamp (>420 nm)100 ml150 min92.6%[60]
g-C3N4/MnO2 /GO (0.5)10 mg L−1300 W Xe lamp (420 nm)100 ml90 min91.4%[61]
Ag3PO4/AgBr/g-C3N4(0.5)40 mg L−1300 W Xe lamp (>420 nm)100 ml25 min80.2%[28]
g-C3N4/Bi2WO6/AgI (0.6)20 mg L−1>420 nm50 ml60 min91.1%[62]
Mn1-CN1 (0.6)20 mg L−1300W xenon lamp50 ml180 min96.97%This study
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Lu, G.; Li, X.; Lu, P.; Guo, H.; Wang, Z.; Zhang, Q.; Li, Y.; Sun, W.; An, J.; Zhang, Z. Z-Type Heterojunction MnO2@g-C3N4 Photocatalyst-Activated Peroxymonosulfate for the Removal of Tetracycline Hydrochloride in Water. Toxics 2024, 12, 70. https://doi.org/10.3390/toxics12010070

AMA Style

Lu G, Li X, Lu P, Guo H, Wang Z, Zhang Q, Li Y, Sun W, An J, Zhang Z. Z-Type Heterojunction MnO2@g-C3N4 Photocatalyst-Activated Peroxymonosulfate for the Removal of Tetracycline Hydrochloride in Water. Toxics. 2024; 12(1):70. https://doi.org/10.3390/toxics12010070

Chicago/Turabian Style

Lu, Guanglu, Xinjuan Li, Peng Lu, He Guo, Zimo Wang, Qian Zhang, Yuchao Li, Wenbo Sun, Jiutao An, and Zijian Zhang. 2024. "Z-Type Heterojunction MnO2@g-C3N4 Photocatalyst-Activated Peroxymonosulfate for the Removal of Tetracycline Hydrochloride in Water" Toxics 12, no. 1: 70. https://doi.org/10.3390/toxics12010070

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics